Reviving Technique:
Reviving technique of IIR bottle stopper trimming or old bottle stopper
First, weigh 100 parts by weight of clean waste IIR bottle stopper trimming, adjust the roll pitch of the refining mill to 0, mill the grinding trimming on the refining mill for 1-2 min, and then add 3 parts by weight of reclaiming agent RDS-IIR, mill for 3 min and add 4-5 parts by weight of paraffin oil, mill run for 6-9 min before sheeting and rolling and the IIR bottle stopper reclaimed rubber is produced.
If there is no refining mill, operate directly on the open mill. First, break the IIR bottle stopper by big roll pitch, and turn the roll pitch to 0.5mm , adding the reclaiming agent RDS-IIR and paraffin oil step by step, mix evenly and turn the roll pitch to 0, sheet after 3 times of mill running.
Physical or Chemical Property of IIR Bottle Stopper Reclaimed Rubber
Test recipe of IIR bottle stopper reclaimed rubber : reclaimed rubber100, accelerator M 0.3, accelerator CZ 0.6, zinc oxide 3, sulfur 1.1.
IIR bottle stopper reclaimed rubber can also be vulcanized by resin or magnesium oxide, etc.
Vulcanizing condition : 170 ℃ X7min
Physical property:
Name |
Hardness / Shore A |
Tensile Strength /Mpa |
National Standard
/Mpa |
Break elongation /% |
National Standard/% |
IIR Bottle Stopper Reclaimed Rubber |
48 |
5.4 |
无 |
580 |
无 |
Storage life: in cool and dry places for 2 years
Package: 25kg /bag